A coil of TA2 titanium arrives at the line with rolling oil and a thin oxide film on its surface. The job is to let chemistry cut the part, not a die. Photochemical etching opens windows in a resist on both faces, and an etchant dissolves the exposed metal. What comes off the line is a flat mesh, a filter screen, or a thin medical shim. Eight steps carry the strip from cleaning to inspection. Each one sets up the next: a dirty surface lifts the resist, a weak exposure softens the edge, and a short etch leaves the holes closed. Titanium is slower to react than stainless steel because of that dense oxide, so the bath and the timing follow the grade and the gauge.

Parameter Window

  • Grades are limited to TA1, TA2, and TC4. TA1 and TA2 are commercially pure; TC4 is stronger and springs back after uncoiling.
  • Strip thickness runs from 0.03 to 2.0 mm. Thin foil wrinkles in transport; thick sheet needs a longer, steadier etch.
  • Resist is dry film or liquid photoresist, applied to both faces. Its thickness has to match the etch depth.
  • The etchant is fluoride based, chosen to break the titanium oxide layer. Temperature and spray pressure follow the grade.
  • Hole and slot size are tied to gauge. Features close to the sheet thickness tend to develop barrel shaped walls.
  • Tolerance depends on part structure. Mesh, slots, and outer contours do not hold the same way under one setup.

Manufacturing Process / Workflow (8 Steps)

  1. Clean — Strip rolling oil, fingerprints, and particles with alkaline and acid washes, then rinse. Titanium oxide must not be stripped too hard, or the resist loses grip.
  2. Apply resist — Laminate dry film or coat liquid resist on both faces. Titanium has low surface energy, so activate the surface first or the film lifts at the edges.
  3. Expose — Copy the artwork onto the resist with aligned tools on both sides. The strip reflects light strongly, so hold vacuum and exposure time steady.
  4. Develop — Wash away the unexposed resist to open the etch windows. Too little leaves skin; too much thins the lines. Check the image before the strip moves on.
  5. Etch — Dissolve the exposed metal until holes and slots break through. This is the step where photochemical etching changes the material. Keep the fluoride bath circulating so reaction products leave the walls.
  6. Strip resist — Remove the coating in an alkaline stripper. Titanium holds residue in recesses, so rinse with warm water before drying.
  7. Clean again — Neutralize and rinse with deionized water, then dry with hot air. Fine slots trap acid, which matters for medical parts.
  8. Inspect — Check through-holes, edge quality, and flatness under a microscope or projector. Tolerance depends on part structure, so set the datum by function.

Core Advantages

On the line, the value of this route shows up in six places:

  1. No hard tool: a design change means new artwork, not a new die.
  2. No press stress: chemical dissolving does not squeeze the metal, so thin sheet stays flat.
  3. No burrs: holes and slots form by dissolution, without the rollover a punch leaves.
  4. Wide gauge range: the same line handles 0.03 mm foil and 2.0 mm sheet.
  5. Free geometry: round holes, long slots, and shaped openings can sit on one part.
  6. Batch repeatability: with fixed exposure and bath state, variation comes mainly from resist thickness.

Typical Applications

  • Titanium mesh for fine sieving and support, with even openings and a flat face.
  • Filter discs stacked into cartridges, where channels must run through cleanly.
  • Medical shims and thin instrument parts that need a clean, stress free surface.
  • Thin heat spreader and shield sheets that rely on flatness and corrosion resistance.
  • Encoder and scale plates whose slots and lines come from exposure, not scribing.
  • Flow control discs for instruments, with hole patterns set by flow demand.

Design Notes & Process Considerations

  1. Set the gauge before the hole: minimum openings move with thickness, and necks under 0.1 mm can be eaten by side etch.
  2. Leave room for alignment: put registration marks outside the hole field.
  3. Round the corners: sharp corners hold resist and collect stress after etch.
  4. Lay out along the rolling direction to limit distortion when the strip is uncoiled.
  5. Coordinate with downstream bending: keep a hole free band along any bend line.
  6. Record grade, gauge, resist thickness, and bath state together, so a later TA1 or TC4 run can be reproduced.
Consult Message